矿产一般工业要求汇编

(据新版规范附录资料汇编)

一、冶金、化工石灰岩及白云岩、水泥原料矿床 ········································· 2 二、岩金矿床及其伴生组分 ············································································ 4 三、铜、铅、锌、银、镍、钼矿床 ································································ 5 四、硫铁矿床 ································································································· 10 五、高岭土、膨润土、耐火粘土矿床 ··························································· 12 六、钨、锡、汞、锑矿床 ·············································································· 14 七、盐湖和盐类矿产 ······················································································ 19 八、磷矿 ········································································································· 21 九、砂矿(金属矿产) ·················································································· 23 十、玻璃硅质原料、饰面石材、石膏、温石棉、硅灰石、滑石、石墨矿 25 十一、重晶石、毒重石、萤石、硼矿 ··························································· 32 十二、铝土矿、冶镁菱镁矿 ·········································································· 36 十三、铁、锰、铬矿 ······················································································ 38 十四、煤矿 ····································································································· 42 十五、稀有金属矿产 ······················································································ 43 十六、稀土矿产 ······························································································ 46 十七、铀矿 ····································································································· 51

1

一、冶金、化工石灰岩及白云岩、水泥原料矿床

(DZ/T0213—2002)

1、黑色冶金熔剂石灰岩化学成分一般要求 类别 石灰岩 白云质灰岩 (高镁石灰岩)

品位界限 边界品位 工业品位 边界品位 工业品位 化学成分质量分子数% CaO ≥48 ≥50 CaO+MgO ≥49 ≥51 MgO ≤3.0 ≤3.0 ≤8.0 ≤8.0 SiO2 ≤4.0 ≤4.0 ≤4.0 ≤4.0 P S ≤0.04 ≤0.15 ≤0.04 ≤0.15 ≤0.03 ≤0.12 ≤0.03 ≤0.12 2、有色冶金熔剂、电石、制碱石灰岩化学成分一般要求 品位界限 边界品位 工业品位 化学成分质量分子数% 冶金熔剂石灰岩 CaO MgO SiO2 ≤2.0 ≤2.0 CaO MgO 电石石灰岩 SiO2 ≤1.0 ≤1.0 R2O3 ≤1.0 ≤1.0 P ≤S ≤CaCO3 ≥88 制碱石灰岩 MgO ≤1.9 ≤1.9 酸不溶物 ≤3.0 R2O3 ≤1.0 ≤1.0 ≥50 ≤1.5 ≥52 ≤1.0 0.06 0.1 ≤≤≥53 ≤1.5 ≥54 ≤1.0 0.06 0.1 ≥90 ≤3.0

3、耐火材料衬炉用、熔剂用白云岩化学成分一般要求 化学成分质量分子数% 品位界限 MgO 边界品位 ≥18 工业品位 ≥20 耐火材料炉衬用白云岩 Al2O3+Fe2O3+Mn3O4+SiO2 ≤3.0 ≤3.0 其中SiO2 ≤1.5 ≤1.5 MgO ≥15 ≥16 熔剂用白云岩 Al2O3+Fe2O3+Mn3O4+SiO2 ≤10 ≤40 其中SiO2 ≤4 ≤4

4、冶金用石灰岩粒度要求 用途 烧结 炼铁

2

粒度范围 mm ≤3 15-60 最大粒度 mm ≤6 ≤80 允许波动的范围 % 上限 ≤10 ≤10 下限 ≤6 5、冶金用白云岩粒度要求 粒度mm 0-5 5-20 10-40 40-80 30-100 块度(mm)限制,所占比例(%) 最大不大于6,大于5的不大于5% 最小不小于3,小于3的不大于10%;最大不大于25,大于20的不大于5% 最小不小于8,小于10的不大于10%;最大不大于45,大于40的不大于5% 最小不小于30,小于40的不大于10%;最大不大于100,大于80的不大于10% 最小不小于20,小于30的不大于10%;最大不大于120,大于100的不大于10% 6、水泥用石灰质原料矿石化学成分一般要求 化学成分质量分子数% 类别 Ⅰ级品 Ⅱ级品 CaO ≥48 ≤45 MgO ≤3 ≤3.5 K2O+Na2O ≤1.6 ≤0.8 SO3 ≤1 ≤1 fSiO2 石英质 ≤6 ≤6 燧石质 ≤4 ≤4

7、粘土质、硅质原料矿石化学成分一般要求 化学成分 类别 粘土质原料 硅酸率(SM) ≥3~4 2~<3 铝氧率(AM) 1.5~3.5 不限 MgO ≤3% K2O+Na2O ≤4% SO3 ≤2% SiO2 ≤80% 硅质原料 MgO ≤3% K2O+Na2O ≤2% SO3 ≤2% 一类 二类 注:SM=ω(SiO2)/ω(Al2O3+Fe2O3),AM=ω(Al2O3)/(Fe2O3) 注:当采用预热器窑和预分解窑时,要求水泥石灰质原料、粘土质原料、硅质原料中氯质量分数不大于0.015%。

8、矿山露天开采技术条件一般要求

项目 最低可采标高 剥采比 可采厚度 夹石剔除厚度 采场最终边坡角 采场最终底盘 最小宽度 爆破安全距离 要求 一般不低于矿区附近的最低地平面标高,如低于最低地平面标高,必须通过技术经济论证确定 覆盖层、脉岩、夹层、边坡围岩的剥离总量与矿石总量之比,一般不大于330.5﹕1(m/m) 石灰岩、白云岩:大、中型矿床一般8m,小型矿4m;粘土质原料、硅质原料:岩石状矿石一般4m,松软状矿石一般1.5m 岩石状矿一般2m,松软状矿石一般1m 岩石状矿一般50o-60o,松软状矿一般45o 岩石状矿:大中型一般不小于60m,小型矿床一般不小于40m;松软状矿:大中型一般不小于40m,小型矿床一般不小于20m 矿床开采边界对公路、铁路、高压线、居民区和其他主要建筑物的爆破安全距离一般不小于300 m,如爆破安全距离小于300 m时,应与投资者商定 3

二、岩金矿床及其伴生组分

(DZ/T0205—2002)

1、岩金矿工业指标参考表 项 目 边界品位 (质量分子数) 最低工业品位 (质量分子数) 矿床平均品位 (质量分子数) 最低可采厚度 夹石剔除厚度 无矿段剔除标准

-6指 标 (1×10)~(2×10),堆浸氧化矿石为(0.5×10)~(1×10) (2.5×10)~(4.5×10) (4.5×10)~(5.5×10) 0.8~1.5 m,陡倾斜者为下限,缓倾斜至水平为上限 2~4 m,地下开采者为下限,露天开采者为上限 对应工程为10~15 m 不对应工程为20~30m -6-6-6-6-6-6-6

2、岩金矿共生(铜、铅、锌)矿产工业指标一般要求表 项 目 边界品位(ωB)% 最低工业品位(ωB)% 矿床平均品位(ωB)% 最低可采厚度m 夹石剔除厚度m

硫化矿石 0.2~0.3 0.3~0.5 0.4~0.5 0.7~1 1~2 2~4 0.7~1 6 1~2 2~4 0.5~1 1~2 6 1~2 2~4 0.5 0.7 1 2 氧化矿石 0.5~1 1.5~2 10~12 1~2 2~4 1.5~2 3~6 10~12 1~2 2~4 Cu(铜) Pb(铅) Zn(锌) Cu(铜) Pb(铅) Zn(锌)

3、岩金矿伴生组分评价参考表 元 素 质量分数 元 素 质量分数

4

铜 Cu 0.1% 砷 As 0.2% 铅 Pb 0.2% 碳 C 锌 Zn 0.4% 硫 S 2% 三氧化钨 WO3 0.05% 钴 Co 0.01% 锑 Sb 0.4% 银 Ag 2(g/t) 钼 Mo 0.01% 三、铜、铅、锌、银、镍、钼矿床

(DZ/T0214—2002)

1、矿床工业指标制订的一般原则

◆矿床工业指标是正确估算和评价矿床的矿产资源/储量的标准和基础。其制订方法有价格法、方案法、类比法、地质统计学方法等。方案法虽然工作量大,但由于其可靠实用而常常被采用;地质统计学方法易于进行多方案比较,选择最佳方案。工业指标制订应结合预可行性或可行性研究进行。制订工业指标的时间应是在野外地质勘探工作基本结束、评价矿床所需的绝大部分原始数据、试验结果已经获得的条件下进行。 ◆预查和普查阶段,评价矿床可使用一般工业指标;详查和勘探阶段,地质勘查部门以一般工业指标为基础,根据具体矿床地质特征确定三至四套试圈指标,以此分别进行矿体圈定和矿产资源/储量试算,形成包括各套方案试算结果、相应的图纸资料在内的工业指标建议书,并将建议书提交负责该项目可行性(预可行性)研究的工业部门或设计研究院。矿山设计研究部门在进行可行性或预可行性研究的同时,负责工业指标各试圈方案的比较工作(可行性研究委托书应包含此内容)。通过资源利用、矿体完整程度、矿床开发经济效益等方面的综合比较,择优确定工业指标方案,并编制工业指标推荐报告,上报有关主管部门批准后正式下达。 ◆用地质统计学方法建立矿床模型、制订工业指标时,应给工业指标制订单位提供记录有钻孔、坑探、槽探测量信息、样品化验分析数据及有关原始资料的软盘或光盘。 ◆制订多组分矿床的工业指标时,应以工业价值占重要地位的组分为主要研究对象,兼顾其他有用组分。对有价值的共生有用组分应同时制订并推荐圈定矿体、估算矿产资源/储量的工业指标。 ◆对矿石中含有的伴生有用组分,应根据具体矿床的地质特征、矿石选(冶)试验结果来确定并推荐评价指标。有时尚需对有害组分的最大允许含量做出规定。

2、铜矿床工业指标一般要求表 项目 边界品位(ωB)% 最低工业品位(ωB)% 矿床平均品位(ωB)% 最低可采厚度m 夹石剔除厚度m

硫化矿石 坑采 0.2~0.3 0.4~0.5 0.7~1.0 1~2 2~4 露采 0.2 0.4 0.4~0.6 2~4 4~8 氧化矿石 0.5 0.7 1 2

5

3、铜矿床伴生有用组分评价参考表 组分 质量分数% 质量分数g/t Pb Zn Mo Co WO3 Sn Ni S 1 Bi 0.05 Au 0.1 Ag 1 Cd、Se、Te、Ga Ge、Re、In、Tl >0.001 0.2 0.4 0.01 0.01 0.05 0.05 0.1

4、铅锌矿床工业指标一般要求表 项 目 边界品位(ωB)% 最低工业品位(ωB)% 矿床平均品位(ωB)% 最小可采厚度m 夹石剔除厚度m

硫化矿石 Pb 0.7~1 5~8 1~2 2~4 Zn 1~2 Pb 0.5~0.7 1~1.5 6~9 1~2 2~4 0.3~0.5 0.5~1 混合矿 Zn 0.8~1.5 2~3 氧化矿石 Pb 0.5~1 1.5~2 1~2 2~4 Zn 1.5~2 3~6 10~12 5、铅锌矿床伴生有用组分评价参考表 组分 质量分数 % 质量分数g/t 组分 质量分数 % 质量分数g/t

Cu WO3 Sn Mo 0.02 Ga Bi 0.02 Ge S 4 Se Sb 0.4 Te CaF2 5 Tl Au 0.1 Hg Ag 2 U 0.06 0.06 0.08 As Cd In 0.02 0.01 0.001 0.001 0.001 0.001 0.001 0.001 0.005 0.02 6、镍矿床工业指标一般要求表 硫化镍矿 项 目 边界品位(ωB)% 最低工业品位(ωB)% 矿床平均品位(ωB)% 最小可采厚度m 夹石剔除厚度m

原生矿石 坑采 0.2~0.3 0.3~0.5 0.8~2 1 ≥2 露采 0.2~0.3 0.3~0.5 0.6~1 2 ≥3 氧化矿石 坑采 0.7 1 1.5 1 ≥2 露采 0.7 1 1.2 2 ≥3 氧化镍— 硅酸镍矿 0.5 1 1 1~2 7、镍矿床伴生有用组分评价参考表 元素 质量分数g/t 质量分数 %

Pt、Pb 0.08 Os、Ru、Rh、Ir 0.02 Au 0.05~0.1 Ag 1.0 Co Se Te 0.01 0.0006 0.0002 6

8、钼矿床工业指标一般要求表 项 目 边界品位(ωB)% 最低工业品位(ωB)% 矿床平均品位(ωB)% 最小可采厚度m 夹石剔除厚度m

硫化矿石 露采 0.03 0.06 0.08~0.1 2~4 4~8 坑采 0.03~0.05 0.06~0.08 0.1~0.12 1~2 2~4 9、钼矿床伴生有用组分评价参考表 组分 质量分数% 质量分数g/t WO3 0.06 Cu 0.1 Pb 0.2 Zn 0.4 Fe 10 S 1 Bi 0.03 Re 10 10、银矿床工业指标一般要求表 项 目 边界品位 g/t 最低工业品位 g/t 矿床平均品位 g/t 最小可采厚度m 夹石剔除厚度m 指 标 40~50 80~100 >150 0.8~1 2~4 11、银矿床伴生有用组分评价参考指标表 元素 质量分数% 质量分数g/t Au 0.1 Pb 0.2 Zn 0.4 Cu 0.1 S 2 Cd 0.005 Mn 4 12、伴生有用组分评价参考指标表说明 A:矿石中伴生元素质量分数大于表中指标时,应研究回收利用途径; B:表中“S”质量分数指标系指黄铁矿中硫在矿石中的质量分数; C:伴生元素中的Cu、WO3、Pb、Zn、Sn、Mo、Fe、Bi、CaF2、Sb等主要是对能形成独立的有用矿物、通过选矿能选成单独精矿产品的,如: ——Pb、Zn、Cu主要指赋存于硫化矿物中者; ——WO3主要指赋存于白钨矿、黑钨矿中者; ——Sn主要指赋存于锡石中者; ——Mo主要指赋存于辉钼矿中者; ——CaF2主要指赋存于萤石中者; ——Sb主要指赋存于硫锑铅矿和脆硫锑铅矿中者; ——Fe主要指赋存于磁铁矿中者; ——Bi主要指赋存于辉铋矿中者; D:Ge、Ga、In、Se、Te、Cd等分散元素,经选矿一般富集在铜、铅、锌的精矿中,通过冶炼回收。

7

13、铜精矿质量标准 品级 一级品 二级品 三级品 四级品

Cu质量分子数不小于 % 30 25 20 13 杂质质量分子数不大于 % As 0.05 0.20 0.30 0.40 Pb+Zn 2 5 8 12 Mg 1 3 4 5 Bi 0.05 0.20 0.30 0.50 注:铜精矿中金、银、硫为有价元素,应报分析数据 14、铅精矿质量标准 品级 一级品 二级品 三级品 四级品

Pb质量分子数不小于 % 70 65 55 45 杂质质量分子数不大于 % Cu 1.2 1.5 2.0 2.5 Zn 4 5 6 7 As 0.2 0.3 0.4 0.6 MgO 1.0 1.5 1.5 2.0 Al2O3 2.0 2.5 3.0 4.0 注:铅精矿中金、银为有价元素,应报分析数据;其他类型铅精矿的杂质要求由供需双方商定 15、锌精矿质量标准 品级 一级品 二级品 三级品 四级品 Zn质量分子数不小于 % 55 50 45 40 杂质质量分子数不大于 % Cu 0.8 1.0 1.0 1.5 Pb 1.0 1.5 2.0 2.5 Fe 6 8 12 14 As 0.2 0.4 0.5 0.5 SiO2 4.0 5.0 5.5 6.0 注:1、铅精矿中银、硫为有价元素,应报分析数据;2、锌精矿中镉、氟质量分数应分别不大于0.3%,锑质量分数应不大于0.03%,锡质量分数应不大于0.1%,镍和锗质量分数要求,由供需双方商定;3、四级品铁闪锌矿含铁允许量不大于18%

16、银精矿质量标准 ◆银精矿质量标准尚未颁布,目前按原中国有色金属工业总公司(1988)中色财字第0596号文:“暂定银大于3000g/t的精矿为银精矿,含银1000~300 g/t的铜、铅精矿为银铜、银铅混合精矿”的规定执行

8

18、钼精矿质量标准(GB3200-89) 牌号 KmO53-A KmO53-B KmO51-A KmO51-B KmO49-A KmO49-B KmO47-A KmO47-B KmO45-A KmO45-B Mo质量分子数不小于 % 53 53 51 51 49 49 47 47 45 45 杂质质量分子数不大于 % SiO2 6.5 5.0 8.0 5.5 9.0 6.5 11.0 7.5 13.0 8.5 As 0.01 0.05 0.02 0.10 0.03 0.15 0.04 0.20 0.05 0.22 Sn 0.01 0.05 0.02 0.06 0.03 0.06 0.04 0.07 0.05 0.07 P 0.01 0.02 0.02 0.03 0.03 0.04 0.04 0.05 0.05 0.07 Cu 0.15 0.20 0.20 0.40 0.22 0.60 0.25 0.80 0.28 1.20 Pb 0.15 0.30 0.18 0.40 0.20 0.60 0.25 0.65 0.30 0.70 CaO 1.50 2.00 1.80 2.00 2.20 2.00 2.70 2.40 3.00 2.60 WO3 0.05 0.25 0.06 0.30 — — — — — — Bi 0.05 0.10 0.06 0.15 — — — — — — 注:1、牌号中的A表示单一钼矿浮选产品;B表示多金属矿综合回收浮选产品;2、钾、钠的质量分数,报分析数据,不作质量分数考核指标;如需方对牌号中未规定的三氧化钨和铋的质量分数有要求,可由供需双方商定;3、经供需双方协议,可调整表中个别指标;4、钼精矿中铼为有价元素,供方应报出分析数据,是否计价,供需双方协议。

9

四、硫铁矿床

(DZ/T0210—2002)

1、矿床工业指标制订的一般原则

◆硫铁矿一般工业指标是供预查、普查阶段圈定矿体、估算资源量的参数依据。 ◆在硫铁矿短缺又急需地区,可根据矿床的开采方式,选矿难易程度、共伴生矿产或组分的综合利用情况等因素,在宏观经济效益允许的条件下,其最低工业品位及可采厚度可适当降低。 ◆有害组分超过最大允许含量的矿石,应单独圈出其范围,供工业部门采取措施处理利用。 ◆当硫铁矿矿石中伴生有硫酸盐类矿物(明矾石、石膏、重晶石等)时,则矿石品位应剔除这部分的含硫量。 ◆其他金属和非金属矿床中的伴生硫,应注意综合评价和综合利用(伴生硫的含量一般达到多少才能综合利用,根据具体矿床研究确定)。 2、硫铁矿一般工业指标参考表

项 目 硫(S)边界品位[ω(S)、%] 硫(S)最低工业品位[ω(S)、%] 最低可采厚度m 夹石剔除厚度m 砷(As)[ω( As)、%] 有害组分最大允许含量 氟(F)[ω( F)、%] 铅锌(Pb+Zn)[ω( Pb+Zn)、%] 碳(C)[ω( C)、%] 硫铁矿矿石品级划分 Ⅰ级品(S)[ω(S)、%] Ⅱ级品(S)[ω(S)、%] Ⅲ级品(S)[ω(S)、%] 指标 8 14 0.7~2.0 1~2 0.1(酸洗流程)或0.2(水洗流程) 0.05(酸洗流程)或0.1(水洗流程) 1 5~8 ≥35 25~35 14~25 3、硫铁矿伴生有益组分综合评价指标参考表 组分 Cu Au Se 综合评价指标 0.1~0.3% 0.3~0.5g/t ≥0.001% 组分 Pb Ag Te 综合评价指标 0.2~0.4% 5~20g/t ≥0.005% 组分 Zn Co Cd 综合评价指标 0.4~0.8% 0.01~0.02% ≥0.01% 注1:本指标是对硫铁矿矿石加工利用时可以随硫精矿富集或能选出独立精矿的,或能富集于其副产品中的矿种(元素)而言 注2:对Cu、Pb、Zn等可通过选矿富集回收者,宜采用指标的下限 注3:矿石中其他组分达到一定含量,并能回收利用的,亦应进行综合评价

10

4、硫铁矿技术指标 指 标 含量(ωB)% 优-Ⅰ 有效硫(S) 砷(As) 氟(F) 铅锌(Pb+Zn) 碳(C) ≤2.0 ≥38 优等品 优-Ⅱ ≥35 ≤0.05 ≤0.05 ≤1.0 ≤3.0 ≤5.0 一等品 ≥28 ≤0.10 ≤0.10 合格品 合-Ⅰ ≥25 ≤0.15 合-Ⅱ ≥22 注1:各组分含量均以干基计。 注2:合—Ⅱ仅适用于煤系沉积硫铁矿。 注3:多金属硫铁矿砷的技术指标按合同执行。 注4:水分是计量依据,技术指标由供需双方议定。 注5:粒度应小于或等于250 mm。

5、硫精矿技术指标 指 标 含量(ωB)% 优-Ⅰ 有效硫(S) 砷(As) 氟(F) 铅锌(Pb+Zn) 碳(C) ≥48 ≤0.05 ≤0.05 ≤0.5 ≤1.0 优等品 优-Ⅱ ≥45 一等品 ≥38 ≤0.07 ≤0.07 ≤1.0 ≤2.0 合格品 ≥28 ≤0.10 ≤0.10 注1:各组分含量均以干基计。 注2:多金属硫精矿砷的技术指标按合同执行。 注3:水分是计量依据,技术指标由供需双方议定。

11

五、高岭土、膨润土、耐火粘土矿床

(DZ/T0206—2002)

1、高岭土一般工业指标 化学成分质量分子数 % 矿石 类型 原矿或 淘洗精矿 Al2O3 Fe2O3+TiO2 总质量分 数 沉积型 硬质 高岭土 原 矿 热液蚀变型原矿 软质 高岭土 原 矿 原 矿 砂质 高岭土 淘洗精矿 -325 目水筛 >24 <2.5 <0.7 >15 >30 <2 其中TiO2 <0.6 淘洗率 % 最低可采厚度m 露天开采 小型矿山 0.7 中型以上矿山 0.7~1 地下开采 夹石剔除厚度m 露天开采 小型矿山 0.3 中型以上矿山 0.3~0.5 地下开采 0.7 0.3 >18 <2 <0.6 >24 >14 <2 <2 <0.6 <0.6 0.7~0.2 2 1 1 2 1

2、膨润土矿一般工业指标 项 目 矿石质量指标 边界品位 蒙脱石质量分数≥40%(单样) 工业品位 蒙脱石质量分数≥50%(单工程) 注:对选矿性能良好,适用于作精细加工产品的低电荷型(怀俄明型)的膨润土,其蒙脱石的质量分数指标可适当降低

3、膨润土矿开采技术条件

项目 矿层最小可采厚度 夹石最小剔除厚度 露天开采标高 露天剥采比 露天矿床最终边坡角 露天开采最终底盘最小宽度

12

要求 1~2 m 不小于1 m 一般不低于采区侵蚀基准面以下50 m 不大于4﹕1 一般50~60o 不小于20 m

4、耐火粘土一般质量要求 矿石类型 矿石品级 特级 Ⅰ级 高铝粘土 Ⅱ级 甲 乙 主要化学成分质量分子数% Al2O3 ≥85 ≥80 ≥70 ≥60 ≥50 ≥44 ≥40 ≥35 ≥30 ≥35 ≥30 ≥25 ≥30 ≥26 ≥22 Fe2O3 ≤2.0 ≤3.0 ≤3.0 ≤3.0 ≤2.5 ≤1.2 ≤2.5 ≤3.0 ≤3.5 ≤2.0 ≤2.5 ≤3.5 ≤2.0 ≤2.5 ≤3.5 CaO ≤0.6 ≤0.6 ≤0.8 ≤0.8 ≤0.8 烧失量% ≤15 ≤15 ≤15 ≤15 ≤15 ≤15 ≤15 ≤15 ≤15 ≤16 ≤16 ≤16 ≤18 ≤18 ≤18 耐火度℃ ≥1770 ≥1770 ≥1770 ≥1770 ≥1770 ≥1750 ≥1730 ≥1670 ≥1630 ≥1690 ≥1670 ≥1630 ≥1670 ≥1610 ≥1580 ≤2.5 1~2.5 化学成分以生料计 化学成分以熟料计 可塑性 指标 备注 Ⅲ级 特级 硬质粘土 Ⅰ级 Ⅱ级 Ⅲ级 半软质 粘土 Ⅰ级 Ⅱ级 Ⅲ级 Ⅰ级 软质粘土 Ⅱ级 Ⅲ级 开采技矿层最小可采厚度:地下开采0.8 ~l m;露天开采0.5 ~0.8 m;夹石最小剔除厚度33术条件 不小于0.5 ~0.8 m;剥采比≤15 m/m。

13

六、钨、锡、汞、锑矿床

(DZ/T0201—2002)

1、钨矿床一般工业指标参考表

项目 边界品位ω(WO3)% 最低工业品位ω(WO3)% 可采厚度m 夹石剔除厚度m 要求 0.06~0.1 0.12~0.20 ≥1~2 ≥2~5 坑采厚度小于0.8米时应 考虑米百分值计算 备注

2、钨矿床伴生有用组分综合评价参考表

组分 (ωB)% 含量 Cu 0.05 Pb 0.2 Nb2O5 0.02 Zn 0.5 Tr2O3 0.03 Sn 0.03 Ga Mo 0.01 Ge Bi 0.03 Cd Sb 0.5 In Co 0.01 S 4 BeO 0.03 Li2O 0.3 组分 Ta2O5 (ωB)% 含量 0.01 Aug/t Agg/t 0.1 1 0.001 0.001 0.002 0.001

3、锡矿床一般工业指标参考表

项目 边界品位ω(Sn)% 最低工业品位ω(Sn)% 可采厚度m 夹石剔除厚度m 要求 0.1~0.2 0.2~0.4 ≥0.8~1 ≥2 坑采厚度小于0.8米时应考虑米百分值计算 备注 注1:本参考指标是以全锡计算,适用于以锡石为主的矿床。当矿床中胶态锡、硫化锡所占比例>l0%时,要提高指标。 注2:以胶态锡、硫化锡为主的矿石,要按采、选、冶技术经济条件另行制定指标。

4、锡矿床伴生有用组分综合评价参考表

组分 质量分数 % Cu 0.2 Pb 0.5 Zn 0.8 Bi 0.01 W 0.02 Mn 4 Fe 20 S 10

14

5、汞矿床一般工业指标参考表

项 目 边界品位ω(Hg)% 最低工业品位ω(Hg)% 可采厚度m 夹石剔除厚度m 要 求 0.04 0.08~0.10 ≥0.8~1.2 ≥2~4 注l:由于汞矿勘查时只能圈出含矿体,上述指标则用于勘查工程中圈定见矿厚度,并据以计算含矿系数及矿体平均品位。 2:评价含矿体时,按含矿系数与品位乘积提出指标要求,即含矿系数×矿体平均品位≥0.04%。 3:指标中品位下限用于规模较大,开采建设条件较好的汞矿床。 4:厚度下限用于陡倾斜矿床,反之则用上限。 5:厚度<0.8m,用米百分值(厚度×品位)确定指标。 6:矿床的平均品位应大于0.12~0.15%,才宜进一步工作。

6、锑矿床一般工业指标参考表

项 目 边界品位ω(Sb)% 最低工业品位ω(Sb)% 可采厚度m 夹石剔除厚度m 要 求 0.5~0.7 1.0~1.5 ≥0.8~1 ≥2 注:当厚度小于0.8米时,按米百分值计算

7、锑矿床伴生有用组分综合评价参考表

组 分 As Au Ag WO3 Hg Bi 质量分数 0.2 % 0.1×10 2×10 0.05 % 0.005 % 0.05 % -6-6组 分 Se Co Ni CaF2 BaSO4 质量分数 0.001 % 0.01 % 0.1 % 5 % 8 %

15

八、磷矿

(DZ/T0209—2002)

1、磷矿一般工业指标参考表 项 目 边界品位(P2O5)% 最低工业品位(P2O5)% 磷块岩矿石品级 (P2O5)% 可采厚度m 夹石剔除厚度m Ⅰ Ⅱ Ⅲ 类 别 磷块岩矿 ≥12 15~18 ≥30 <30~24 <24~15 1~2 1~2 磷灰岩矿或磷灰石矿 5~6 10~12 备注 适合擦洗脱泥的风化矿石,Ⅰ级品的P2O5可降低到28% 注:1、表中所列是指以钙磷酸盐为主的矿石类型,对于其他磷酸盐矿物新类型矿石,要根据选矿加工试验另行确定;2、缺磷地区工业指标,可根据矿床的开采方式、选矿难易程度、共伴生矿产或组分的综合利用情况和矿肥结合等因素考虑,在宏观经济效益允许的条件下,其边界品位和最低工业品位可适当降低;3、可采厚度和夹石剔除厚度因矿体赋存条件和矿床开采方式不同而定,缓倾斜矿床的可采厚度一般不小于1.5 m,富矿或陡倾斜矿床可采厚度可适当降低,露天开采矿床的可采厚度、夹石剔除厚度可适当增大。 2、酸法加工用磷矿石标准 项目 ω(P2O5)% ≥ ω(MgO)/ω(P2O5)% ≤ ω(R2O3)/ω(P2O5)% ≤ ω(CO2)% ≤ 优等品 Ⅰ 34.0 2.5 8.5 3.0 Ⅱ 32.0 3.5 10.0 4.0 Ⅰ 30.0 5.0 12.0 5.0 一等品 Ⅱ 28.0 10.0 15.0 7.0 合格 等品 24.0 注:1、水分以交货地点计,质量分数应小于或等于8.0%;2、除水分外各组分质量分数以干基计; 3、当指标中仅MgO/P2O5或R2O5/P2O5一项超标,而另一项较低时,允许MgO/P2O5的指标增加(或减少)0.4%,但此时,R2O5/P2O5指标应减少(或增加)0.6%;4、什邡式磷矿石合格品的五氧化二磷质量分数应大于或等于26.0%;5、合格品中杂质要求按合同执行。 3、黄磷用磷矿石标准 项目 ω(P2O5)% ≥ ω(SiO2)/ω(CaO)% ≥ ω(CO2)% ≤ 粒度mm 注:各组分质量分数以干基计

21

优等品 30.0 — 一等品 28.0 6.0 合格等品 Ⅰ 26.0 0.2 Ⅱ 24.0 0.4 5~50(小于5mm的不超过5%)

4、钙镁磷肥用磷矿石标准 项目 ω(P2O5)% ≥ ω(MgO)% ≥ ω(R2O3)% ≤ 粒度mm 4.0 优等品 28.0 — 8.0 一等品 24.0 合格等品 20.0 1.0 — 15~100(小于15mm的不超过5%) 注:1、各组分质量分数均以干基计;2、五氧化二磷质量分数大于或等于19.0%、18.0%、17.0%,对应的氧化镁质量分数分别大于或等于3.0%、5.0%、7.0%的磷矿石可作为合格品;3、电炉法、旋风炉法等用磷矿石技术指标,可由供需双方参照本标准议定

5、钙镁磷肥用硅镁质半自溶性磷矿石标准 项目 ω(P2O5)% ≥ ω(MgO)% ≥ ω(SiO2)% ≤ ω(Al2O3)% ≤ 18.0 3.5 合格等品 16.5 4.5 12.0~32.0 3.0 15~100(小于15mm的不超过5%) 15.5 4.5 注:l、各组分质量分数均以干基计;2、未加工的矿石粒度指标,可由供需双方协商议定;3、电炉法、旋风炉法等用磷矿石技术指标,可由供需双方参照本标准议定

6、磷肥放射性镭-226限量卫生标准(GB 8921—88) 序号 标 准 1 磷肥中226Ra的含量不得高于500 Bq·kg-l 为了保证磷肥中226Ra符合1项限量标准,用于生产磷肥的磷矿石226Ra含量不2 应超过500 Bq·kg-1 产品天然铀含量的检验结果若低于30×10-6,即可认为该产品符合1项的要求,3 不再作镭-226的测定 新建、扩建磷矿山必须向当地放射卫生防护部门提交有关226Ra含量的地质报4 告,经复查符合GB 8921—88标准后方可投产

22

九、砂矿(金属矿产)

(DZ/T0208—2002)

1、金红石及钛铁矿砂矿一般工业指标参考表 砂矿名称 金红石(矿物) 钛铁矿(矿物) 边界品位kg/m 1 10 3最低工业品位kg/m 2 15 3可采厚度m 0.5 ≥0.5~1 夹石剔除厚度m (剥采比≤4) ≥0.5~1 2、砂锡矿一般工业指标参考表 项目 边界品位 最低工业品位 可采厚度m 夹石剔除厚度m 用化学方法确定品位(锡石中锡) Sn的质量分数0.02% Sn的质量分数0.04% ≥0.5 ≥2 用淘洗法确定锡石含量 (锡石纯度:Sn的质量分数≥60%) 锡石100~150g/m 锡石200~300g/m ≥0.5 ≥2 33注:化学方法确定品位多用于残坡积砂矿;淘洗法确定锡石含量用于河流砂矿 3、砂金矿一般工业指标参考表 露天开采 全面开采 项目 南方 50~100L 混合砂边界品位g/m 混合砂块段最低工业品位g/m 最小可采厚度m 无矿地段(夹石)剔除宽度m 矿体最低可采砂矿量万m 砂矿层边界品位g/m 最低工业品位g/m 砂矿层采幅高度m 33333采掘船开采 北方(含高寒地区) 50~100L 0.06~0.08 0.18~0.20 30~35 30~35 100~300 150~300L 0.05~0.07 0.16~0.18 40~60 40~60 600~1400 水枪开采 0.1 0.3 20 分别 开采 地下 开采 150~300L 0.04~0.06 0.14~0.16 40~60 40~60 900~2000 0.05~0.07 0.16~0.18 30~35 30~35 150~450 0.3~0.5 0.6~1.0 1 3 1.3~1.5 4、稀有金属与稀土金属砂矿一般工业指标参考表 项目 边界品位g/m 最低工业品位g/m 矿块最低工业品位g/m 矿床最低品位g/m 可采厚度m 夹石剔除厚度m

3333绿柱石(手选) 铌铁矿、褐钇铌矿 600 2000~2500 1 5~50 20~250 ≥0.5 (剥采比1﹕1)2 锆石英 独居石 磷钇矿 ≥50 1 2 23

1000~1500 100~200 30~50 4000~6000 200~250 ≥0.5 280~500 500 ≥0.5 1~2 5、重砂矿物分离质量要求简表 项 目 区域普查的自然重砂 重矿物应富集至50~70%,不淘掉目的矿物,重矿物损失率不超过2% 重矿物部分,质量0.1g以上者,纯度一般大于90%; 轻矿物部分,重矿物含量小于同级重矿物总量的2% 样品粒度相差悬殊时,应酌情分级 样量在15 g以下者,一般不缩分,15 g以上者酌情缩分,每次缩分允许差小于0.2 g; 详查、勘探自然重砂,样量大于200 g者,每次缩分允许差小于0.5 g; 样量小于200 g者,每次缩分允许差小于0.2 g; 为寻找贵金属、金刚石的样品一般不缩分 用l/10天平称量,允许差小于天平感应量的2倍 样品称量要求同上; 分离后各部分称量用l/100或1/1 000天平;贵金属、金刚石用1/10万天平称量; 允许差小于天平感应量的2倍 磁性与非磁性矿物应基本分开,各部分分离纯度应在95%以上(非磁性矿物具有磁铁矿包裹体或连生体者除外) 分选级数应视电磁部分的矿物组合、含量等因素而定,电磁性部分的纯度应在95%以上(非电磁性矿物具有电磁性矿物包裹体或连生体者除外),无电磁性部分含电磁性矿物不能超过1% 详查、勘探的自然重砂 重矿物富集应大于70%,尾砂中含重矿物不超过0.5%,砂金、铂等贵金属矿、金刚石不得遗漏 尾砂中含重矿物小于同级重矿物总量的1%,样品损耗率小于1% 室 内 淘 洗 粗淘 精淘 筛分 缩分 重砂总重 称 重 鉴定样品及分离后样品称重 磁 选 电磁选 注:1、样品的总损耗率小于3%;2、贵金属和金刚石在各个工序均不应遗漏;3、小于0.074 mm粒级矿物精淘纯度一般不低于80%,但对于定量分析样品应采取多种手段提高其纯度;4、样品的分选,以提纯目的矿物为原则,其主要部分尽可能富集到同级目的矿物总量的80%以上,磁选、电磁选的损耗率分别小于1%

24

十、玻璃硅质原料、饰面石材、石膏、温石棉、硅灰石、

滑石、石墨矿

(DZ/T0207—2002)

1、玻璃硅质原料矿石类型

◆玻璃硅质原料矿石分为岩类矿和砂类矿两类: 岩类矿包括海相沉积的石英岩、石英砂岩及热液成因的脉石英等;砂类矿包括海相沉积石英砂,河流相沉积含长石、粘土石英砂,湖相沉积含长石、石英砂等

2、平板玻璃用硅质原料质量要求 化学成分% 级别 优等品 一级 二级 三级 四级 粒度组成不大于(%) ω(SiO2) ω(Al2O3) ω(Fe2O3) +1mm +0.8mm +0.71mm +0.5mm -0.1mm 不少于 不大于 不大于 98.50 98.00 96.00 92.00 90.00 1.00 1.00 2.00 4.50 5.50 0.05 0.10 0.20 0.25 0.33 0 0.50 0 0.50 5.50 5.00 10.00 20.00 25.00 30.00 注:1、优等品+0.5mm粒级含量不大于5.5%,包括+0.71mm粒级;2、各级产品的水分要求不大于5%;3、各级产品化学成分的允许波动值:优等品SiO2土0.20%,A12O3土0.10%,Fe203土0.01%;一级品Si02±0.25%,A12O3土0.15%;二级品SiO2士0.30%,A12O3土0.20%;三、四级品Si02土0.30%,A1203土 0.30%;4、矿石中含铬铁矿、铬尖晶石、锆英石、夕线石等难熔矿物时,常使玻璃出现黑点,目前成品平板玻璃中每平方米允许黑点数有限制,在评价矿石质量时应注意对难熔矿物含量和粒度的评价;5、达不到要求需要选矿的矿石,其原矿的质量要求可根据选矿试验结果或与有类比条件矿山类比确定。采用水洗样评价矿石质量时,应根据水洗试验或选矿试验结果,经技术经济论证后确定原矿质量要求或水洗砂质量及含砂率要求

3、器皿玻璃用硅质原料质量要求 含量% 等级 ω(SiO2) ω(Al2O3) ω(Fe2O3) ω(Cr2O3) Ⅰ Ⅱ Ⅲ >99 >96 >90 <1.0 <2.0 <4 <0.05 <0.1 <0.35 <0.001 说明 玻璃仪器器皿玻璃(不包括晶质玻璃) 一般器皿玻璃、无色玻璃 用于一般瓶罐玻璃

4、玻璃硅质原料开采技术条件要求

25

矿床类型 可采厚度m ≥2 0.5~1 夹石剔除厚度m >0.5~1 >0.5 平均剥采比 ≤0.5﹕1 1﹕1 露天矿场最小底盘宽度m ≥40 露天矿场 边坡角大于100m时为50~55o;小于100m时为55~60o 30o 爆破安全 距离m 一般≥400 岩类矿床 砂类矿床 5、饰面石材矿石类型

◆饰面石材矿是指具有一定的装饰性能、物理化学性能、加工性能和能加工成一定尺寸规格的岩石,主要用于建筑物的内外表面装饰。目前中国商业上的天然饰面石材主要有大理石和花岗石两类: ◆大理石类饰面石材大多属于沉积的碳酸盐岩和与之有关的变质岩(如大理岩、蛇纹石化大理岩等),较适用于室内装饰; ◆花岗石类饰面石材大多属于各种产出的岩浆岩(花岗岩、辉长岩、闪长岩、斑岩等)和变质的含硅酸盐矿物为主的岩石(如片麻岩、混合岩等),可适用于室内外装饰。

6、饰面石材矿石装饰性能的一般要求

◆饰面石材矿石的装饰性能表现为经加工后具有一定的颜色、花纹和光泽度,而这些与其物质成分(主要是矿物成分)、结构、构造有关,商业上根据饰面石材的颜色、花纹差异划出不同品种和不同档次。一般较好的(中档以上的)饰面石材经加工后,拼装在一个装饰面上能显现出颜色纯正、花纹和谐、光泽度高。 ◆饰面石材中的色斑、色线影响装饰性能,在荒料、板材的标准中均有限制;石材中的空洞也影响装饰性能(有时可通过某些措施予以弥补),碳酸盐岩石材中的石英、燧石除可能影响装饰性能外,最主要的是对加工性能有影响。石材中存在的某些金属硫化物、泥质物、有机物等,由于易于风化而影响石材的装饰性能和耐久性,因此含这些杂质较多的石材一般不宜用于室外装饰。 ◆由于目前还没有划分饰面石材品种和档次的明确标准,市场对饰面石材的需求常因人、因地、因时、而异,因此,对于勘查的饰面石材品种,应由勘查投资者确定,并与地质勘查单位共同选定标准样,以此作为鉴定勘查矿石品种的依据。

7、饰面石材矿荒料率的一般要求

◆饰面石材荒料是指具有一定块度的直角六面体。对于年产3000m3以上饰面石材荒料的矿山的荒料块度一般可划分为三类,即:I类荒料块度大于等于3m3,Ⅱ类荒料块度大于等于1 m3,Ⅲ类荒料块度大于等于0.5 m3。一般要求荒料的边长不小于0.5 m,3中档和一般档次饰面石材的荒料块度大于1 m。 ◆饰面石材矿的荒料率是指从开采的总体积与所获得的荒料体积的百分比,一般要求中档饰面石材的荒料率不小于20%,在其他技术经济条件相近的情况下,对于高档饰面石材矿的荒料率要求可相应降低,对一般的饰面石材的荒料率要求可相应提高。 ◆荒料率(%)=获得的荒料体积(m3)÷开采的总体积(m3)×100%。

8、饰面石材板材率的一般要求

26

◆饰面石材矿板材率是指荒料经加工后所获得的具有一定尺寸规格的抛光的板材面积,通常以m3/m3表示。一般要求中档饰面石材的板材率不小于18(m3/m3);在其他技术经济条件相近的情况下,对于高档饰面石材矿的板材率要求可相应降低,对一般档次的饰面石材矿的板材率可相应提高。 ◆板材率(m3/m3)=获得的具有一定尺寸规格的抛光的板材面积(m3)/被加工荒料的体积(m3)。

9、饰面石材矿山开采技术条件一般要求

可采厚度m 夹石剔除厚度m 最低开采标高 不低于当地侵蚀基准面,如在技术经济可行条件下,可相应降低侵蚀基准面 露天矿场 边坡角 岩石状岩体50-90o,松散状岩体不大于45o 露天矿场最小底盘宽度m 剥采比 33m/m 视矿山开采总的经济效益而定 3 ≤30~40 10、石膏矿石主要类型

类型 大类 亚类 纤维石膏 石膏: [石膏/(石膏+硬石膏)] ≥石膏(石膏≥硬石膏) 硬石膏-石膏: 50%≤[石膏/(石膏+硬石膏)]<75% 75% 巨-伟晶石膏 石膏 泥质石膏 (粘土质石膏) 碳酸盐质石膏 硬石膏-石膏 泥质石膏-硬石膏 (粘土质硬石膏 -石膏) 碳酸盐质硬石膏-石膏 石膏-硬石膏 泥质石膏-硬石膏 (粘土质石膏 -硬石膏) 碳酸盐质石膏-硬石膏 硬石膏: [石膏(石膏+硬石膏)]<25% 硬石膏 泥质硬石膏 (粘土质硬石膏) 碳酸盐质硬石膏 石膏、硬石膏 硬石膏(+石膏)>85% 硬石膏 硬石膏 碳酸盐 粘土矿物 碳酸盐 硬石膏、石膏 粘土矿物 石膏、硬石膏 硬石膏-石膏:(石膏+硬石膏)>85% 碳酸盐 矿石不经选矿 石膏、硬石膏 粘土矿物 矿石的主要矿物成分 膏矿物 石膏 石膏 石膏(+硬石膏)>85% 石膏 石膏 石膏、硬石膏:(石膏+硬石膏)>85% 杂质矿物 粘土矿物 碳酸盐 备注 石膏需经选矿获得 石膏需经选矿获得或矿石不经选矿 石膏-硬石膏: 25%≤[石膏/硬石膏(石膏<硬石膏) (石膏+硬石膏)]<50% 11、石膏矿一般工业指标

27

类型 层状石膏、硬石膏矿 工业品位(ωB)% 矿石可采厚度m 露天开采 2 地下开采 1 夹石剔除厚度m 露天开采 2 地下开采 1 CaSO4·2H2O+ CaSO4≥55 CaSO4·2H2O≥95 纤维石膏矿 线含矿率14,其中纤维石膏可采单层(脉)厚度2cm 纤维石膏CaSO4·2H2O≥95 层状石膏、硬石膏矿CaSO4·2H2O+ CaSO4≥55,综合线含矿率(γx+κγc)≥14,其中 1.7 纤维石膏及层状石膏、 硬石膏矿 可采单层(脉)厚度:层状石膏、硬石膏10cm,纤维石膏2cm,γx为纤维石膏线含矿率,γc 1.7 1 为层状石膏、硬石膏线含矿率,κ(折合系数)=(层状石膏、硬石膏生产成本或售价)/纤维石膏生产成本或售价,建议κ值采用0.2 松散层中巨-伟晶石膏矿 CaSO4·2H2O≥85 含矿率要求根据选矿试验确定 2 2 注:1、对质量较低的矿石,应充分考虑开采贫化的影响,相应提高矿石品位要求;2、对以硬石膏为主的矿床,应根据不同用途进行工业利用试验,确定工业指标

12、温石棉矿一般工业指标

类型 边界品位(含棉率)(ωB)% ≥0.5 工业品位(含棉率)(ωB)% ≥1.4 矿石可采厚度m 0.5(当厚度小于0.5m,品位大于1.4%,可按米百分值计) 1(当厚度小于1m,品位大于1.5%,可按米百分值计) 夹石剔除厚度m 0.5 镁质碳酸盐岩型矿床 镁质超基性岩型矿床 ≥0.6 ≥1.5 1 注:对某些石棉纤维性能好,具备短纤维湿纺工艺利用性能的,其工业指标按矿床实际情况确定 13、温石棉纤维长度分级标准及纤维组成 等级或 级别 手选1级 手选2级 机选3级 机选4级 机选5级 机选6级 平均纤维长度不小于mm 19 9 平均纤维含量% 60 60 +12.5mm 12~65 0 0 0 干式分级% 不小于 +4.75mm 24~55 10~60 0 0 +1.4mm 8~25 30~70 50~80 20~40 不大于 满底 3~8 10~20 20~50 60~80 含砂量不大于% 5.0 10.0 0 0.3 0.5 1.0 夹杂物含量 % 不大于 0.04 0.04 0.02 0.02 14、温石棉各级纤维质量指标表

28

等级或 级别 手选1级 手选2级 比表面积dm/g 湿式分级% +1.18mm累 计含量不小于 35~55 10~30 5~8 2~4 -0.075mm粉尘含量不大于 32~40 45~55 57~60 65~67 +1.18mm累 计含量不小于 10~30 5~8 2~4 快速湿式分级% -0.075mm粉尘含量不大于 42~52 54~57 62~64 纤维系数 0.7~1.10 0.5~0.6 0.25~0.3 含砂量不大于% 5.0 10.0 0 0.3 0.5 1.0 机选3级 80~120 机选4级 70~120 机选5级 80~120 机选6级 90~100 15、工业应用对硅灰石矿石质量要求 工业用途 质量要求 硅灰石矿按化学成分评价矿石质量时,要求SiO2 38~58%,CaO 36~55%,CO2≤6%,Fe2O3≤1.7%;按矿物组分评价矿石质量时,要求硅灰石含量≥60%(透辉石含量可折抵硅灰石量),石英≤20%,方解石≤13%,Fe2O3≤1.7%。按化学成分或矿物组分提出的工业要求,可任选其一 硅灰石矿要求:SiO2≥49%,CaO≥45%,Fe2O3≤0.2%,325目(0.043 mm)矿粉吸油量20-25 g/100g,水溶物≤0.5%,水萃取pH值7~9,325目(0.043 mm)矿粉白度≥90% 硅灰石精矿质量要求:硅灰石≥50%,方解石≤50%,石英≤5%,S≤0.01%,P≤0.01% 硅灰石精矿质量要求:SiO245~55%,CaO 35~45%,MgO≤8%,S≤0.03%,P≤0.03% 建筑陶瓷用 油漆涂料用 冶金保护渣用 电焊条工业用 16、硅灰石矿矿石质量一般工业指标 矿石可手选矿床 项 目 露天开采 边界品位 工业品位 ≥20~30 ≥25~35 含矿率% 地下开采 ≥25~35 ≥30~40 矿石需机选矿床 硅灰石矿物含量% 露天开采 ≥40 ≥45 地下开采 ≥40 ≥50 注:l、视矿石质量优劣和变化情况以及选矿手段,工业品位可按块段或矿体计算。优质矿石可取下限,质量差的取上限;2、由于硅灰石矿产出特征和当前手选、机选效率、效益存在差别,故机选人选品位高于手选人选品位要求。应根据机选试验成果具体确定;3、手选矿石块度暂按直径大于等于4cm。其质量的最低要求应满足建筑陶瓷用和冶金保护渣用的矿石质量要求

17、硅灰石矿床开采技术条件一般要求 开采方式 可采厚度m 1~2,当矿体真厚度小于露天开采 可采厚度时,可用含矿率米百分值圈定矿体 地下开采 1 1 1~2 夹石剔除厚度m 最低开采 标高 不低于当地侵蚀基准面以下50m 露天矿场边坡角爆破安全距离 在制订勘探矿床工业指标时明确 露天矿场最小底盘宽度m 总剥采比m/ m 33≥20 ≤3﹕1 18、以滑石含量为工业指标矿石质量一般要求

29

品位 边界品位 工业品位 滑石含量ω(B)% ≥35 ≥50 ω(CaO)% 不限 不限 ω(Fe2O3)% ≤3 ≤2 白度 ≥50 ≥60 19、以滑石含量为工业指标矿石工业品级划分 品级 特级品 一级品 二级品 三级品 滑石ω(B)% ≥90 ≥80 ≥70 ≥50 ω(CaO)% ≤1.5 ≤2.5 ≤3.5 不限 ω(Fe2O3)% ≤0.5 ≤1.0 ≤1.5 ≤2.0 白度 ≥90 ≥80 ≥70 ≥60 注:1、品级变化大,不能细分时,可将特、一、二级品合并称富矿,三级品称贫矿;2、三级品滑石矿尚需确定应用方向,对口勘探 20、以化学组分含量为工业指标矿石质量一般要求 品位 边界品位 工业品位 ω(SiO2)% ≥27 ≥36 ω(MgO)% ≥26 ≥27 ω(CaO)% 不限 不限 ω(Fe2O3)% ≤3 ≤2 白度 ≥50 ≥60 注1:只适用于滑石伴生矿物中: A:不存在含镁硅酸盐类矿物,石英含量小于3%; B:含镁硅酸盐类矿物加石英总量小于8%,其中石英含量小于2%; C:含镁硅酸盐类矿物总量小于10%,不含石英的白云石—滑石型、菱镁矿—滑石型矿石。对于含镁硅酸盐类矿物含量超过10%的蛇纹石—滑石型、绿泥石—滑石型、透闪石—滑石型以及成分更复杂的混合类型矿石的工业指标,需根据矿石的具体矿物组成、含量及产品应用方向与勘查投资者具体商定。

21、以化学组分含量为工业指标矿石工业品级划分 品级 特级品 一级品 二级品 三级品 ω(SiO2)% ω(MgO)% ω(CaO)% ≥61 ≥55 ≥48 ≥36 ≥31 ≥30 ≥29 ≥27 ≤1.5 ≤2.5 ≤3.5 不限 ω(Fe2O3)% ≤0.5 ≤1.0 ≤1.5 ≤2.0 白度 ≥90 ≥80 ≥70 ≥60 注1:只适用于滑石伴生矿物中: A:不存在含镁硅酸盐类矿物,石英含量小于3%; B:含镁硅酸盐类矿物加石英总量小于8%,其中石英含量小于2%; C:含镁硅酸盐类矿物总量小于10%,不含石英的白云石—滑石型、菱镁矿—滑石型矿石。对于含镁硅酸盐类矿物含量超过10%的蛇纹石—滑石型、绿泥石—滑石型、透闪石—滑石型以及成分更复杂的混合类型矿石的工业指标,需根据矿石的具体矿物组成、含量及产品应用方向与勘查投资者具体商定。 注2:品级变化大,不能细分时,可将特、一、二级品合并称富矿,三级品称贫矿。 注3:三级品滑石矿尚需确定应用方向,对口勘探。 22、石墨矿一般工业指标

30

类型 晶质(鳞片状)石墨矿 风化矿石 原生矿石 矿石品位(ωB)% 边界品位 2~3 2.5~3.5 ≥55 工业品位 2.5~3.5 3~8 ≥65 可采厚度m 露天开采 2~4 地下开采 0.7~1.4 夹石 剔除厚度m 露天开采 1~4 地下开采 1~3 剥采比 33m/m 不大于 3﹕1~4﹕1 隐晶质(土状)石墨矿 注:由于晶质(鳞片状)石墨的片度不同,其工业用途及经济价值都相差甚大,在制定作为提供矿山建设设计依据的地质勘查报告所用工业指标时,应根据正目石墨含量的高低,提出相应不同高低的边界品位和工业品位要求,即正目石墨含量高时,品位要求可低;反之,则品位要求要高。对应边界品位及工业品位的正目石墨含量要求,一般可掌握在40-60%左右。正目石墨含量是指矿石经选矿所得精矿筛析后,+100(0.147mm)目石墨在精矿中所占的百分比。

31

十一、重晶石、毒重石、萤石、硼矿

(DZ/T0211—2002)

1、钻井液用重晶石粉质量标准 项 目 密度g/cm细度% 3 指标 特级 ≥ 4.30 3.0 5.0 150 110 110 一级 4.20 3.0 5.0 200 125 125 指 标 二级 4.05 3.0 5.0 250 140 140 0.074 mm孔径筛筛余量 ≤ 0.043 mm孔径筛筛余量 ≥ 水溶性碱土金属(以钙计)mg/kg ≤ 粒度效应 加硫酸钙前 ≤ mPa.s 加硫酸钙后 ≤ 2、化工用重晶石质量标准 项 目 优-1 硫酸钡(BaSO4)含量 % 二氧化硅(SiO2)含量 % 爆裂度 % ≥95.0 ≤3.0 ≥60 优等品 优-2 ≥92.0 一等品 ≥88.0 ≤5.0 合格品 ≥83.0 — — 注:各组分含量以干基计;合格品的二氧化硅和爆裂度指标按供需合同执行 3、化工用毒石质量标准 项 目 质量分子数(ωB)% BaCO3 >36% R2O3 <1.5% CaO <7% 化学成分 % 品级 特二级 特一级 一级品 二级品 三级品 四级品 五级品 六级品 七级品 ω(CaF2),≥ 98.0 97.0 95.0 90.0 85.0 80.0 75.0 70.0 65.0 杂质,≤ ω(SiO2) 1.5 2.5 4.5 9.0 14.0 18.0 23.0 28.0 32.0 ω(S) 0.05 0.08 0.10 0.10 0.15 0.20 0.20 0.25 0.30 ω(P) 0.03 0.05 0.06 0.06 0.06 0.08 0.08 0.08 0.08 不溶性滤渣(主要由BaSO4组成) <56% 4、萤石块矿化学成分质量标准 注:1、产品粒度:6~300 mm,小于6 mm的产品不得超过5%,大于300 mm的产品不超过10%,不允许有大于350mm的产品;2、萤石块矿中不得混入泥土、废石等外来杂质。3、对萤石块矿产品另有要求时,由供需双方协商解决;4、该标准适用于冶金等行业使用的萤石块矿

32

5、橡胶、造纸填充料用重晶石粉质量标准 项 目 质量分子数(ωB)%

BaSO4 >98 CaO <0.36 R2O3(Fe2O3、Al2O3) 微量 不许有锰、铜、铅等杂质 6、萤石粉矿化学成分质量标准 品级 特三级 特二级 特一级 一级品 二级品 三级品 四级品 五级品 六级品 七级品 八级品 化学成分% ω(CaF2),≥ 98.0 97.0 95.0 90.0 85.0 80.0 75.0 70.0 60.0 50.0 40.0 Ⅰ 0.2 0.2 0.3 — — — — ω(Fe2O3),≤ 0.2 0.2 0.2 0.2 Ⅱ 0.3 0.3 注:1、表中“—”表示含量不规定;产品粒度:6~0mm,根据不同粒度有具体要求时由供需双方协商解决;2、萤石粉矿中不得混入杂质;3、该标准适用于陶瓷、搪瓷、玻璃、水泥等行业使用的萤石粉矿

7、氟石精矿化学成分质量标准 化学成分 % 品级 特级 一级品 二级品 三级品 四级品 ω(CaF2),≥ 98 97 95 93 杂质,≤ ω(SiO2) 0.6 0.8 1.0 1.4 2.0 ω(CaCO3) 0.7 1.0 1.2 1.5 — ω(S) 0.03 — — — — ω(P) 0.02 — — — — 注:表中“—”表示含量不规定;用户对杂质含量有特殊要求时,可由供需双方协定;干态氟石精矿中水质量分数不得大于0.5%;湿态氟石精矿中水质量分数不得大于10%;氟石精矿的粒度,要求通过0.154 mm孔径网筛(-100目)的质量不小于87%;氟石精矿中不得混入外来杂物

33

8、硼镁石矿石质量标准 等级 指标名称 三氧二化硼(B2O3)质量分数% ≥ 全铁(以Fe2O3计)质量分数% ≤ 氧化钙(以CaO计)质量分数%≤ 氧化镁(以MgO计)质量分数%≤ 矿石块度mm < 注:各项成分含量均以干基计 优等品 24 22 一等品 20 18 8 45 400(300-400mm的不大于15%,小于20mm的不大于15%) 二等品 16 15 14 三等品 Ⅲ-2 10 12 优-1 优-2 Ⅰ-1 Ⅰ-2 Ⅱ-1 Ⅱ-2 Ⅲ-1

9、重晶石矿(原生矿)一般工业指标 项目 边界品位 最低工业品位 最低可采厚度 夹石剔除厚度

指标 ω(BaSO4) ≥30% ω(BaSO4)≥50% 0.80~1.50 m l ~2 m

10、重晶石矿(残、坡积矿)一般工业指标 项目 含矿率 最低可采厚度 剥采比

指标 ≥0.5 t/m3 [ω(BaS04)≥45%] ≥0.30 m ≤1 11、毒重石矿一般工业指标 项目 边界品位 最低工业品位 最低可采厚度 夹石剔除厚度

指标 ω(BaCO3)≥20% ω(BaCO3)≥36% 0.80 m 1 m 12、萤石矿床一般工业指标 项目 边界品位 最低工业品位 富矿:ω(CaF2)≥65% ω(S)<1% 贫矿:ω(CaF2)20~65%

34

指标 ω(CaF2) ≥20% ω(CaF2) ≥30% 最低可采厚度 夹石剔除厚度 最低可采厚度 夹石剔除厚度 0.7 m 0.7 m 1.0 m 1~2 m 13、硼矿床一般工业指标 项目 边界品位 最低工业品位 最低可采厚度 夹石剔除厚度 露天剥采比:3~6 m3/m3 注:富矿:B2O3>11%,可直接加工利用的矿石 贫矿:B2O35~11%,需经选矿(或作配矿)才能利用的矿石 指标 ω(B2 O 3)=3% ω(B2 O 3)=5% 1~2 m 1 ~2 m

35

十二、铝土矿、冶镁菱镁矿

(DZ/T0202—2002)

1、铝土矿床一般工业指标 一水硬铝石型 项目 露采 边界品位 块段最低工业品位 铝硅比值 ω(Al2O3)% 铝硅比值 ω(Al2O3)% 1.8~2.6 ≥40 ≥3.5 ≥55 0.5~0.8 0.5~0.8 10~15 广西某地堆积型 一水硬铝石型 2.6 ≥40 ≥3.8 ≤0.3 ≤1.5 ≤1.3 ≤0.6 暂不限 ≥0.5 ≥0.5 ≥200 ≥300 ω(Al2O3)% 铝硅比值(A/S) ω(Al2O3)% S 有害组分最大允许 含量ωB% CaO+MnO CO2 P2O5 有机质 最低可采厚度m 夹石剔除厚度m 剥采比m3/m3 边界含矿率km/ m3 矿区(段)平均矿率km/ m3 沉积型矿床 坑采 1.8~2.6 ≥40 ≥3.8 ≥55 0.8~1.0 0.8~1.0 海南某地红土型 三水铝石型 2.1~2.6 ≥28 ≥0.2 12~15 ≥30 最低可采厚度m 夹石剔除厚度m 剥采比m3/m3 2、堆积型与红土型铝土矿参考工业指标 项 目 边界品位 块段最低工业品位 铝硅比值(A/S) 3、冶镁菱镁矿主要参考工业指标 项目 ω(MgO)% ω(CaO)% ω(SiO2)% 最低可采厚度m 夹石剔除厚度m

矿石级别 特级品 ≥47 ≤0.6 ≤0.6 一级品 ≥46 ≤0.8 ≤1.2 二级品 ≥45 ≤1.5 ≤1.5 2~4 1~2 36

三级品 ≥43 ≤1.5 ≤3.5 四级品 ≥41 ≤6.0 ≤2.0

4、铝土矿用作电熔刚玉原料时的质量要求 项目 ω(Al2O3)% ω(Fe2O3)% ω(SiO2)% ω(TiO3)% ω(CaO)% ω(CaO+ MgO)% ω(烧失量)% 铝硅比值(A/S) 进厂块度 mm 烧失率 %

第二砂轮厂 ≥85 <5 <5.6 3.5~6.5 <0.4 <0.5 ≥15 <250 第四砂轮厂 ≥80 <6 <5.5 <1.2 <1 ≥12 20~300 <4 注:l、一水硬铝石型铝土矿;2、熟料;3、供矿品位 5、铝土矿用作高铝水泥原料时的质量要求 项目 ω(Al2O3)% ω(TiO3)% ω(Fe2O3)% ω(TiO3)% 铝硅比值(A/S)

郑州水泥厂 >72 <6 <2 >7 浙江萧山炼铁厂 >70 <6 <1.5 <4 >7 注:l、一水硬铝石型铝土矿;2、生料;3、供矿品位 37

十三、铁、锰、铬矿

(DZ/T0200—2002)

1、炼钢用铁矿石一般工业指标 矿石类型 磁铁矿石 赤铁矿石 ω(TFe) ≥56% 主要有害物质 ω(SiO2) ≤13% ω(S) ≤0.15% ω(P) ≤0.15% 其他有害物质 ω(Cu)≤0.2% ω(As)≤0.1% 注:矿石块度要求平炉用铁矿石25-250mm;电炉用铁矿石50-100mm;转炉用铁矿石10-50mm 2、炼铁用铁矿石一般工业指标 矿石类型 ω(TFe) 主要有害物质 ω(SiO2) ω(S) ω(P) 其他有害物质 ω(Cu)≤0.2% ω(Pb)≤0.1% ω(Zn)≤0.1% ω(Sn)≤0.08% ω(As)≤0.07% ω(F)≤1.0% 磁铁矿石 赤铁矿石 褐铁矿石 菱铁矿石 ≥50% ≤18% ≤0.30% ≤0.25% 注1:褐铁矿石、菱铁矿石为扣除烧损后折算的标准;自熔性矿石全铁质量分数[ω(TFe)]可降至≥40%。磷含量为一般要求,按炼铁品种不同对矿石含磷量要求也不同:酸性转炉炼钢生铁矿石ω(P)≤0.03%;碱性平炉炼钢生铁矿石ω(P)≤(0.03~0.18%);碱性侧吹炉炼钢生铁矿石ω(P)≤(0.2~0.8%);托马斯生铁矿石ω(P)≤(0.8~1.2%);普通铸造生铁矿石ω(P)≤(0.05~0.15%);高磷铸造生铁矿石ω(P)≤(0.15~0.6%)。注2:矿石块度要求:8~40mm。 3、需进行选矿的铁矿石一般工业指标 矿石类型 磁铁矿石 赤铁矿石 菱铁矿石 褐铁矿石 ω(TFe)% 边界品位 ≥20 ω(mFe)≥15 ≥25 ≥20 ≥25 工业品位 ≥25 ω(mFe)≥20 28~30 ≥25 ≥30 注:如果矿石易采、易选,经济效果好,或含有可以综合回收的伴生组分,则全铁(TFe)含量要求可适当降低;磁铁矿石中硅酸铁、硫化铁、碳酸铁含量较高,则采用磁性铁(mFe)标准。 4、矿床开采技术指标 矿床开采技术指标 最小可采厚度m 夹石剔除厚度m

露天矿 2~4 1~2 坑内矿 1~2 1 38

5、铁矿石中伴生组分评价参考含量表 伴生组分 V2O5 TiO2 Co Cu Ni Pb Zn Sn 质量分数 0.15~0.20% 5% 0.02% 0.1~0.2% 0.1~0.2% 0.2% 0.5% 0.1% 伴生组分 Mo S P2O5 Nb2O5 TR2O3 U An Ag 质量分数 0.02% 2~4% 1~2% 0.05% 0.5% 0.005% (0.1~0.3%)×10-6 5×10-6 注:表中Co、Cu、Ni、Pb、Zn、Mo、S、Au、Ag系指这些元素赋存于硫化物中的质量分数;V2O5指赋存于有用铁矿物中的质量分数;P2O5指磷灰石状态时的质量分数;U指以晶质铀矿、方钍石等独立矿物存在时的质量分数;Nb2O5指以铌铁矿矿物为主的质量分数;TR2O5指以独居石、氟碳铈矿矿物为主时的质量分数;Sn指富集在铁精矿中的锡,当铁精矿还原焙烧时,锡被挥发,可在烟道中回收或在铁尾矿中呈锡石单独矿物的质量分数;TiO2指钒钛磁铁矿床中,可被选出的粒状钛铁矿中的质量分数;铁矿石中其他有用组分,如铬、镓、锗、硼等达到多少质量分数即可综合回收,目前尚无成熟经验,在工作中可据具体情况与有关部门商定;表中质量分数一般为块段平均品位。

6、冶金用锰矿石一般工业指标 自然工业品类型 分类 级 Ⅰ 富锰Ⅱ 矿石 Ⅲ 贫锰矿石 铁锰Ⅱ 矿石 Ⅲ 富锰矿石 贫锰矿石 铁锰矿石 含锰矿石 Ⅰ ω(Mn)% 边界 品位 10~15 10 10 10 8 单工程平均品位 40 35 30 18 25 20 15 25 15 15 12 ω(Mn+ Fe)% ≥50 ≥40 ≥30 ≥25 ω(Mn)/ ω(Fe) ≥6 ≥4 ≥3 ≥3 每1%锰 允许含磷量% ≤0.004 ≤0.005 ≤0.006 ≤0.2%(磷总量) ≤0.2%(磷总量) ≤0.2%(磷总量) ≤0.005% ≤0.2%(磷总量) 碱性矿石 ω(SiO2)% ≤15 ≤25 ≤35 ≤25 ≤25 ≤25 ≤25 ≤35 氧化锰矿石 碳酸锰矿石 注:1、灰质氧化矿石(脉石以方解石为主,碱度≥0.8,烧失量质量分数达18%以上)的评价,可采用碳酸锰矿石的工业指标;2、自熔性、碱性的锰矿石,可酌量降低其富矿锰晶位指标;3、当碳酸锰矿石的灼失量较高,虽然锰的质量分数略低于25%,但焙烧后锰含量可达到氧化锰富矿矿石标准时,这类碳酸锰矿石也可作为富锰矿石考虑。 矿床开采技术指标:矿层最低可采厚度0.5~0.7m;夹石剔除厚度0.2~0.3m;堆积矿净矿含矿率(质量分数)≥15%。

39

7、优质锰矿石、优质富锰矿石品位及杂质含量指标 工业分类 品级 自然类型 氧化锰矿石 碳酸锰矿石 氧化锰矿石 碳酸锰矿石 氧化锰矿石 碳酸锰矿石 ω(Mn)% ≥18 ≥15 ≥35 ≥28 ≥30 ≥25 ω(Mn)/ ω(Fe) ≥6 ≥6 ≥6 ≥6 ≥4 ≥4 ω(P)/ ω(Mn) ≤0.003 ≤0.003 ≤0.003 ≤0.003 ≤0.005 ≤0.005 烧失量 ≥20% ≥20% ≥20% 优质锰矿石 Ⅰ Ⅱ 优质富锰 矿石 注:优质锰矿石、优质富锰矿矿层最低可采厚度标准可为0.3-0.4 m

8、锰矿石中伴生组分评价参考含量表 元素或 组成 含量ωB Co 0.02~ 0.06% Ni 0.1~ 0.2% Cu 0.1~ 0.2% Pb 0.4% Zn 0.7% Au 0.2×10-6% Ag (5~ 10)×10-6 B2O3 1~3% S 2~4% 注:锰矿石中伴生元素多呈细微粒分散、包裹,或与锰、铁矿物组合的状态出现

9、天然放电镁(镁粉)一般技术指标 品级 Ⅰ Ⅱ Ⅲ Ⅳ Ⅴ

ω(MnO2)% ≥75 ≥70 ≥65 ≥60 ≥55 ω(TFe)% ≤2.8 ≤3.5 ≤4.5 ≤5.5 ≤6.5 制成锰粉的放电时间min ≥570 ≥510 ≥450 ≥390 ≥330 注:其他有害元素一般标准为:ω(Cu)<0.0l%,ω(Ni)<0.03%,ω(Co)<0.02%,ω(Pb)<0.02%。

10、化工用二氧化锰矿粉一般技术要求 用 途 制硫酸锰 制高锰酸钾

40

ω(MnO2) ≥50% ω(Fe) ≤3% ≤5% ω(SiO2) ≤5% ω(A12O3) ≤3% ≤4% ω(CaO) ≤0.5% ω(MgO) ≤0.1%